TiN average settings markdown
Beliaev2023
30W at 20ubar 50+11 sccm Lower to reach 4ubar While Ramp DC from 30W to 350W at 5W/sec 5 mins of pre-sputtering Deposition rate was: 0.2nm/s at 200C and room temp, 0.18nm/s at 400C or slower at 600C
What I did
(Average substrate temperature: to add -> it was the only main factor between #8 and #9)
#1 First i did 118nm 12.7 7.8 5.4 - 18 minutes Rate = 0.11 nm/s Colour = Transmissive Blue
#2 start at 7ubar 350W+8.7W 2+2 sccm / 6.6ubar 345W 2+2 sccm During 5mins it was lowered to 4.3 ubar 314 W + 8.7W 1.5+1sccm 2.5 mins at 4.1ubar 350W + 8.7W 1.5+1 sccm 2.5 mins at ~ "" but 2+1 sccm and 400C Final ten seconds ~"" but after heater was on to reach 600C => Measured one at 172nm inferred 172-118=54nm => Measured on glass 90nm -> Rate: 0.29 in 310s upper, 0.18 in 490s lower Rate = 0.17 upper bound, 0.11 lower bound nm/s Colour = Golden
#3 On TiO2 substrate -> Shiny Golden (aimed for 90s, got 310nm if TiO2 was 54nm - which is to be double checked) On 90nm Golden TiN -> Blue (poor uniformity according to profilometer) -> and it this one 176nm in total (~90nm x2 i think so) or is it 176nm ontop of 90nm -> could there have been TiO2 contamination from the other samples to explain blue at this thickness
#3 Settings: 39% power = ? Substrate temp = 400C sccm = 1 Ar + 1 N pressure = 4.5 ubar Time = 7.5 mins / 450 secs thickness golden = 310nm (or incorrect if TiO2 was thicker) thickness blue = 90nm (or 176nm if step was between blue and golden layers) rate golden = 0.69nm/s (too fast??) rate blue = 0.2nm/s (or 0.39nm/s if step was between blue and golden layers)
#4 Simply Uniform Red 175nm Settings: substrate temp = 175C sccm = 1 Ar + 2 N pressure = 4ubar Power was high = 350W Time = 15 minutes / 900 secs Rate = 0.1944 nm/s
#5 Weighted-Average and Error Estimates: Power: Average Power, P̅ = 243 ± 6 W Pressure: Average Pressure, p̅ = 5.26 ± 0.84 μbar Argon Flow: Average Argon Flow, Q̅₍Ar₎ ≈ 1.21 ± 0.08 SCCM Nitrogen Flow: Average Nitrogen Flow, Q̅₍N₎ ≈ 1.11 ± 0.08 SCCM Deposition Rate: Overall Deposition Rate, R₍overall₎ = 0.13 nm/s (from 98 nm in 750 s) Low-pressure Deposition Rate, R₍low-p₎ = 0.20 nm/s (480 s under low-pressure conditions)
Plain Text Markdown TiN #5: Power: 243.2 ± 5.6 W Pressure: 5.26 ± 0.84 μbar Argon Flow: 1.21 ± 0.25 SCCM Nitrogen Flow: 1.11 ± 0.13 SCCM Deposition Rate (overall): 0.13 nm/s Deposition Rate (under 5 μbar): 0.20 nm/s
TiN #6: Power: 297.2 ± 1.0 W Pressure: 4.72 ± 0.16 μbar Argon Flow: 1.55 ± 0.24 SCCM Nitrogen Flow: 1.25 ± 0.09 SCCM Deposition Rate: 0.30 nm/s
TiN #7: (Note: One segment without a power value was omitted from the power average.) Power: 264.4 ± 5.4 W Pressure: 4.80 ± 0.09 μbar Argon Flow: 1.24 ± 0.09 SCCM Nitrogen Flow: 1.36 ± 0.11 SCCM Deposition Rate: 0.06 nm/s
TiN #7.5: Power: 268.7 ± 7.4 W Pressure: 4.81 ± 0.33 μbar Argon Flow: 1.39 ± 0.21 SCCM Nitrogen Flow: 1.33 ± 0.04 SCCM Deposition Rate (overall): 0.11 nm/s Deposition Rate (under 5 μbar): 0.14 nm/s
TiN #8: Power: 297.1 ± 3.81 W Pressure: 4.50 ± 0.15 μbar Argon Flow: 1.36 ± 0.06 SCCM Nitrogen Flow: 1.39 ± 0.05 SCCM Deposition Rate: 0.075 nm/s
TiN #9: Power: 318.4 ± 3.76 W Pressure: 4.75 ± 0.09 μbar Argon Flow: 1.34 ± 0.07 SCCM Nitrogen Flow: 1.35 ± 0.03 SCCM Deposition Rate: 0.25 nm/s